              Extrusion laminating process common problems and solutions

              Extruded composite is a high pressure high temperature rapid processing of plastic process, which links to the machine, a variety of factors raw materials, personnel of each operation. The actual process will be a variety of abnormalities, now on a variety of anomalies will be described.

              Problems CAUSE Solution
              Poor adhesion

              1. The resin surface oxidation is not sufficient

              2. The resin temperature is too low

              3. Composite wheel insufficient pressure

              4. incomplete drying primer low printing ink adhesion

              5. The substrate is abnormal

              6. Check whether the damp substrates

              1.1 increase in resin temperature

              1.2 reduce line speed

              1.3 increase in the air gap distance

              2.1 increase in resin temperature

              2.2 increase backpressure

              2.3 Check the heater

              Composite wheel pressure increase

              4.1 increasing the drying temperature

              4.2 reduce speed

              4.3 to adjust the amount of air intake and exhaust

              Check the base of factor 5.1

              5.2 Check the base with non-polluting

              5.3 Have damp printing ink

              Replacing Ink

              Uneven thickness

              1.T-die temperature is set incorrectly

              2. Composite wheel uneven pressure

              3. foreign matter adhering to die

              4. deflector abnormal

              Re-adjust the temperature

              2.1 composite wheel balance adjustment

              2.2 Replacing the composite wheel

              Shutdown, cleaning die

              4.1 Check the deflector Model

              4.2, lower deflector position adjustment

              Composite wrinkles

              1. Composite wheel roundness bad

              2. The speed is too low

              3. Import wheel imbalance

              The tension is too small

              5. Composite wheel of a foreign body

              6. The original film is the wrong way to wear paper

              Replace or abrasive composites wheel

              Increase recombination velocity

              Import balance wheel adjustment

              Increased tension

              Cleaning of wheel

              Check wear paper mode

              Gel and fish eye pattern

              1. The resin temperature is too low

              2. Resin damp

              To improve resin temperature

              Re-drying resin

              Crystallization point

              1. The resin processing temperature is too high

              2. Replace the resin is not sufficient

              Lower resin temperature

              Replace the resin

              Wrinkles shaft

              1. The winding tension, weakness set improperly

              2. The substrate on both sides of the thick

              Reset tension and weakness
              2.1, trimming
              2.2 Adjust the thickness

              Poor transparency

              1. The temperature of the cooling wheel
              2. The cooling roller surface treatment discomfort, kneading the resin shortage

              2.1, increasing backpressure

              2.2, adjust the temperature

              Shrink film

              1. The resin temperature is too high

              2. The tension of the tension is too large

              3. The composite speed is too low

              4. insufficient cooling cooling wheel

              Lower resin temperature

              Adjust tension

              Increase recombination velocity

              Lowering the cooling temperature

               